A peelable tray seal is a designed failure point. The seal layer is formulated to let go at a predictable force, usually between 2 and 5 newtons per 15 mm strip, while still holding modified atmosphere pressure through a 1,200-mile truck route. Lock-up seals take the opposite position: weld the film to the tray flange so hard that the substrate tears before the bond releases, then let a die-cut corner or a resealable lidding film structure handle consumer access.
Both approaches are legitimate. The decision usually comes down to what the package has to survive and who has to open it.
What Actually Breaks When a Peelable Seal Opens
Peelable systems fail in one of three places, and the mechanism you choose drives both the force curve and the appearance of the flange after opening.
- Cohesive peel: the seal layer splits internally, typically because an incompatible minor phase (polybutene-1 at 10 to 20 percent, or a polypropylene domain in a PE matrix) creates weak planes. Opening force is stable across a wide temperature window but leaves a slightly hazy, fibrous residue on the flange.
- Adhesive peel: the bond between film and tray releases at the interface. Clean appearance, no stringing, but the force is sensitive to seal temperature and any brine or fat contamination on the flange.
- Delamination peel: the seal holds, and a deliberately weak tie layer inside the film splits instead. This gives very consistent forces and is common where a reseal function needs a fresh, uncontaminated surface after the first open.
Lock-up seals skip all of this. The seal layer and the tray are the same or highly compatible resins, so the interface effectively disappears, and the weld strength exceeds the tear strength of the thinner component.
EVA, Metallocene Plastomers and Ionomers Do Different Jobs
Most of the engineering in tray lidding happens in the 8 to 25 micron sealant layer. Three families cover the majority of commercial structures, and they are frequently blended rather than used alone.
EVA: The Low-Cost Workhorse
Ethylene vinyl acetate with 9 to 18 percent VA content gives a seal initiation temperature in the 70 to 90 degree C range and generous tack. It is forgiving on older tray sealers with uneven platen pressure. The trade-off is poorer hot tack under load and a tendency toward higher haze and odor at the upper VA levels, which matters for premium retail trays.
Metallocene Plastomers: Narrow Distribution, Tight Control
mPE plastomers in the 0.880 to 0.902 g/cm3 density band deliver high hot tack with a narrow melting range, which is exactly what you want when a tray sealer gives you 0.5 to 1.2 seconds of dwell. Because the comonomer distribution is uniform, the peel force curve is flatter and batch-to-batch drift is smaller than with conventional LLDPE. Blended at 20 to 40 percent into a peelable masterbatch, they widen the usable seal window by roughly 10 to 15 degrees C.
Ionomers: Seal Through Contamination
Ionomers remain the choice for wet protein, brined cheese, and anything where marinade finds the flange. Seal initiation can start near 60 degrees C, and the ionic clusters let the melt displace liquid and particulate rather than trapping it in the bond line. They are the most expensive of the three per kilogram, so most structures use a thin ionomer skin over a cheaper core instead of a full-thickness layer.
Setting the Burst and Peel Window Before You Specify a Resin
The useful way to brief a film supplier is as a range with two hard edges, not a single target number. A typical fresh-protein tray program might look like this:
- Minimum burst: package survives 0.5 psi internal pressure without seal creep, covering gas flush expansion and the roughly 17 percent drop in external pressure at 5,000 feet of elevation.
- Peel force band: 2.5 to 4.5 N/15 mm at 300 mm/min, measured per ASTM F88 seal strength methodology.
- Seal window: at least 20 degrees C of jaw temperature over which both conditions hold, so a drifting sealer does not produce leakers at shift change.
- Hot tack: enough green strength to hold product weight during the one to two seconds before the flange cools, usually 1.5 to 3 N/25 mm for a 500 g tray.
Human factors research on package opening generally puts comfortable adult opening force well under 50 N of applied effort, and lower still for older consumers, which is why the upper edge of the peel band matters as much as the lower one.
Where a Lock-Up Weld Is Still the Right Answer
Lock-up construction wins when distribution abuse outranks convenience. Think bulk foodservice trays shipped on slip sheets, 5 kg catering portions, long ocean freight with temperature cycling, or retort and pasteurization cycles where internal pressure spikes while the polymer is soft. A properly matched lock seal film on an APET or CPET tray will typically show substrate tear at 15 to 40 N/15 mm rather than any measurable interface release.
Consumer access then comes from a separate feature: a laser score, a die-cut tab, a corner notch, or a perforated opening panel. The cost moves from the resin into the converting step, which is often the cheaper place to put it at high volumes.
Tray Material Narrows the Choice Faster Than Anything Else
Peelability is a two-sided relationship, and the flange resin sets the rules.
- APET and RPET trays: need a peelable sealant with PET affinity, often an ionomer or acrylic-modified blend; raw PE will not bond reliably.
- Polypropylene and CPET: higher sealing temperatures (typically 160 to 190 degrees C jaw) and good candidates for PP-based cohesive peel systems.
- Foam PS trays: limited heat tolerance, so low-seal-initiation EVA or ionomer blends keep the flange from collapsing.
- Mono-material PE trays: attractive for recyclability but prone to lock-up unless a deliberate incompatible phase is formulated into the sealant.
Flange geometry matters too. A 6 mm flat flange with a 0.3 mm radius behaves very differently from a 4 mm flange with a rolled lip, particularly on peel initiation at the corners.
Reseal Adds a Third Performance Requirement
Reseal changes the problem from one event to roughly five to fifteen. The first open has to meet the peel spec, the exposed adhesive has to stay tacky after sitting in a refrigerator at 4 degrees C, and the reclose has to hold enough to keep product from drying out, usually 10 to 25 percent of the original peel force.
Pressure-sensitive adhesive zones, cold-seal patterns, and delaminating tie layers all handle this differently. The failure mode worth testing early is adhesive transfer onto product or onto the consumer’s fingers, because it shows up in reviews long before it shows up in a lab report.
Validation Steps Worth Running Before Commercial Trials
- Seal curve mapping at three temperatures, two pressures, and two dwell times to find the true process window, not just the peak.
- Burst and creep testing per ASTM F1140 and F2054 at ambient and at chilled temperature.
- Opening force on aged samples at 7, 30, and 60 days, since many peel systems drift upward as the blend anneals.
- Contamination challenge: deliberately dose the flange with product fat or brine, then seal and test.
- Food contact confirmation for every layer that touches product, per FDA food contact substance requirements.
Frequently Asked Questions
What Peel Force Is Considered Easy-Open for a Retail Tray?
Most retail tray programs target 2 to 5 N per 15 mm strip measured at 300 mm/min. Below about 2 N, you start risking distribution leakers and premature corner opening, and above roughly 6 N, older consumers and anyone with reduced grip strength begin to struggle.
Can One Film Give Both High Burst Strength and Easy Opening?
Yes, within limits, and that is the whole purpose of a formulated peel layer. Burst resistance comes from seal area, flange width, and the sealant’s resistance to shear creep, while opening force comes from the peel mechanism, so a cohesive peel system can hold 0.7 psi internal pressure and still open at 4 N.
Talk Through Your Seal Specification With RTG Films
Contact RTG Films, send us your tray material, sealer settings, and target peel and burst numbers, and our team will work through sealant options and run seal curve data against your actual conditions. We can sample peelable, lock-up, and resealable structures from the same brief so you can compare them on your own line.